Introduction

Marks on the sheet in the wet end come mainly from the forming section and, even more often, from the press section. The wetter the sheet entering the press (typically 18–22% dryness off the wire), the more easily fiber arrangement is disturbed and marks appear; high press line pressure is another common trigger. This guide summarizes the main types of wet-end marks and their typical causes and remedies.

Part 1: Marks from the Forming Section

1.1 Forming Fabric Marks

These match the fabric weave pattern, sometimes at the same angle on the sheet. Usually caused by an unsuitable fabric type or too-fast dewatering (especially in the initial drainage stage). An unsuitable fabric should be corrected with the supplier's design; excessive dewatering can be reduced by raising beating degree, adjusting the stock landing point, increasing dewatering blade spacing, and tuning suction-box vacuum. Too-low fabric tension can also cause marks — increase it — and avoid pressing the vacuum pickup roll too deep into the forming section.

1.2 Seam Marks

Easy to identify: they cross the full width in a band of about 10 cm, and their spacing matches the fabric length. They relate to the seaming process; most modern fabric makers can resolve this. If not, choose a more suitable supplier.

1.3 Longitudinal Streaks

Caused mainly by local stock clumps at the headbox slice, improper baffle settings, locally worn suction-box covers or stock accumulation, or uneven high-pressure showers. Usually not difficult to fix.

Part 2: Marks from the Press Section

2.1 Felt Base-Fabric Marks

As the surface batt wears and the base fabric becomes exposed, it prints onto the sheet — typically straight, dense, evenly spaced fine stripes along the machine direction, appearing in the mid-to-late felt life. Reduce press line pressure where acceptable; if that fails, replace the felt. Excessive high-pressure shower (worn nozzles, dispersed jets), too-high vacuum, or a rough suction-box cover can accelerate wear and bring on base-fabric marks early — check shower pressure, nozzle condition, vacuum box configuration, and the condition of press and felt rolls.

If regular fine lines appear shortly after a felt is installed, the felt design may be unsuitable (e.g., too-light weight lets excess water through the nip, printing a dewatering mark matching the base yarn density). Remedies: increase batt weight (more wear resistance, higher water content and flow resistance, slower dewatering); increase base fabric weight (more layers, higher yarn density) to cushion pressure; and choose a suitable weave — plain weave shows the heaviest marks, 2/2 broken twill lighter, and 1/3 broken twill lightest.

2.2 Felt Batt-Layer Marks

The press is the highest line-pressure zone in the machine; unsuitable batt selection or poor operation can print batt marks. Viewed obliquely or against back light, they appear as earthworm-like depressions — single-fiber or twisted multi-fiber marks — and can occur at any stage of felt life. Early-life marks mean the batt is too coarse; mid-to-late marks mean the fine surface batt is worn and the middle batt is exposed.

To reduce them, the felt maker can use finer surface batt, increase the amount of surface batt, add low-melt bicomponent fiber (fused in finishing for wear resistance), and singe the surface to remove loose fiber. Operators should install the felt in the marked running direction (arrow) — especially important for seamed felts, since batt orientation is set during needling and finishing; fully wet a new felt to avoid dry abrasion; control high-pressure water pressure and suction-box vacuum; ensure the high-pressure needle covers the full width in one traverse for even washing without gaps or overlap; and make sure the low-pressure fan showers ahead of the suction boxes cross-cover.

2.3 Vacuum Roll Marks

On 3-roll 2-nip or 4-roll 3-nip combined presses, the sheet often shows marks matching the vacuum press roll's hole pattern. During vacuum dewatering, fines and fillers concentrate in the hole zones, producing higher opacity. Machine measures: change the press configuration (e.g., 4-roll 3-nip to 5-roll 3-nip), lower line pressure, reduce vacuum. Felt design: use a multi-layer base with larger-diameter base yarns for rigidity and a bridging effect, raising void volume and compressibility.

2.4 Shower Water Streak Marks

Uneven high-pressure showers make felt moisture uneven, so nip dewatering is inconsistent and streaks print on the sheet. These can only be solved by strengthening on-site machine management.

2.5 Press Dewatering Marks

As water is squeezed into the felt and transferred to rolls or the shoe, marks appear — fine, straight, regular marks along the machine direction or regular hole-like marks. These may be base-fabric, vacuum-roll, blind-drilled-roll, grooved-roll, or grooved-shoe marks.

Higher line pressure pushes more water through the felt and makes marks more likely, especially in mid-to-late felt life. To distinguish base-fabric from groove marks, count marks per centimeter and match against base yarn density or groove density (base yarn density is usually higher).

Remedies: (1) increase felt weight at high-pressure nips (e.g., shoe press) or high-dewatering positions (e.g., first press), and balance the batt-to-base ratio and base selection by speed and line pressure; (2) choose press roll material and groove/blind-hole design appropriately — reducing groove width or hole diameter lowers the risk; (3) if marks occur, reduce machine speed and line pressure; (4) for high-speed fine paper, a lightweight nonwoven felt is the best choice — a 1+1 base (nonwoven top layer plus a single-layer woven base) balances dewatering needs against flow resistance, and additional batt weight also helps. Ensuring adequate sheet dryness off the wire is equally key to avoiding excessive press dewatering demand.

Conclusion

Wet-end marks have many causes, so solutions must match the actual situation. On-site machine management is critical, and felt manufacturers should strengthen on-site observation, understand machine characteristics in depth, and supply products that truly match the paper machine.